Production Process for Copper-Aluminum Tube Welding Lines

Aug 11, 2026

Leave a message

Pre-welding Preparation
This step is crucial for ensuring effective filler metal wetting and directly determines joint quality:

‌Joint Preparation‌: The copper tube is machined into a socket configuration to receive the aluminum tube; the radial clearance is strictly controlled between 0.05 and 0.2 mm, and the joint overlap length does not exceed 30 mm (butt joints are avoided).
‌Copper Surface Activation‌: Sanding with 120-grit abrasive paper removes the oxide layer, ensuring a surface roughness of Ra ≤ 1.6 μm; this is followed by a 2-minute immersion in a 5% sulfuric acid solution to form a CuSO₄ transition layer.
‌Aluminum Surface Roughening‌: Degreasing via alkaline washing in a 10% NaOH solution at 60°C for 3 minutes, followed by acid pickling in a mixture of 20% HNO₃ and 5% HF for 1 minute to break down the high-melting-point Al₂O₃ oxide film and create a microscopically rough surface.

 

Filler Metal Placement and Fixture Positioning
A "sandwich" composite filler structure is employed to inhibit the formation of brittle phases:

An Al-Si-Cu-Ni series filler metal (such as 4047 Al-Si alloy) is used in conjunction with a 0.1 mm thick copper foil interlayer, with the melting point controlled between 560°C and 580°C.
The filler metal ring or strip is positioned in the welding zone with a gap of ≤0.05 mm against the tube's outer wall; the inner diameter of the filler ring is 0.3 mm larger than the tube's outer diameter to ensure uniform heating and melting.